PETG Pellet Drying Before Injection Molding or Extrusion
PETG dries at 65–70 °C for three to six hours in air at −20 °C dew point. Most PETG drying failures are air problems, not temperature problems.

PETG dries at 65–70 °C for 3 to 6 hours in air at a dew point of −20 °C or lower, down to about 0.05 % residual moisture. That window covers unfilled copolyester pellets for injection molding and for extrusion. Thick-wall and optical parts often want 0.02 %, which is the same temperature with longer time and drier air, not a hotter dryer.
The temperature is the easy part. Air is the hard part. Almost every PETG drying problem we are asked to solve turns out to be an air problem wearing a temperature costume.
65 to 70 °C is a heat-margin number, not a drying number
The ceiling comes from the resin's glass transition, which for PETG sits around 80 °C. A dryer set to 78 °C to push material through faster softens the pellets resting against the hopper wall. Softened pellets flatten, stick together, and bridge into a plug that someone has to dig out with a spatula at three in the morning.
Ten degrees of margin. That is the whole reason the number looks low next to PET, which is routinely dried at 150 °C and above because its pellets are semi-crystalline and hold their shape. PETG is amorphous, so the pellet itself gives way as it approaches Tg.
The floor has a reason too. At 55 °C the bed climbs to temperature slowly and three hours is not enough for a 200 kg charge. So the window is narrow from both sides, and neither side is negotiable with a bigger heater.
The air can carry more water than the pellets will surrender
Plant air at 25 °C and 60 % relative humidity carries about 12 g of water per kilogram of dry air. Heating that air to 70 °C removes no water at all; it only drops the relative humidity reading. Air from a desiccant dryer holding a −20 °C dew point carries roughly 0.6 g/kg, and a −40 °C dew point gets you to about 0.08 g/kg.
That is a twentyfold difference in how much water the process air can take away, and it explains how "we ran it six hours" and "it still splays" live comfortably in the same building.
A hot-air hopper dryer fed on ambient air tends to level off somewhere above 0.1 % on PETG, because the air reaching the pellets is close to balance with them. More hours do not fix that. Drier air does.
Sizing the hopper from the shot weight
Here is the calculation the temperature table never gives you.
A press running a 300 g shot, part plus runner, on a 25-second cycle consumes 43 kg/h. At 4 hours of drying, 173 kg of PETG has to be sitting at 65–70 °C at any given moment rather than passing through. PETG pellets bulk at roughly 0.8 kg/L, so 173 kg occupies about 216 L of working volume.
Now check what you were about to order. A 150 L machine-side hopper holds about 120 kg, which at 43 kg/h gives 2.8 hours of residence — the bottom edge of the window, and outside it the moment the shot weight or the cycle time changes. A 300 L vessel looks comfortable until you measure the band between the low-level probe and the high-level probe, because 216 L is 72 % of nameplate and most hoppers do not offer that much usable band once the cone and the space above the high mark are excluded. Ask for working volume at your fill levels and the answer will be smaller than the catalog.
One more consequence worth naming: if the same press runs two grades, the hopper has to be emptied between them, and 173 kg is how much material you scrap per changeover.
Extrusion, regrind, and the grades that leave the window
Extrusion is easier to size and harsher on exposure. Draw is steady, so a sheet line running 400 kg/h with a 4-hour requirement needs 1.6 t of dried inventory ahead of the die, all of it at temperature, and a line that stops for a screen change leaves that inventory cooking with nothing coming out of the far end.
Regrind deserves its own sentence. Ground PETG sheet and trim carry more surface area and usually more moisture than virgin pellet, at the same setpoint, so a blend above roughly 20 % regrind means the drying time that worked on virgin resin is no longer the drying time you need.
Then there is the grade itself. PETG is a family, not a molecule: copolyester grades with a different comonomer ratio, plus glass-filled and flame-retardant compounds, can carry their own window. And a supplier sheet that says "4 hours at 65 °C" usually assumes desiccant air even when it does not say so. That omission is the common one, and it is the reason a shop can follow a data sheet exactly and still mold wet parts.
What we can and cannot tell you from a data sheet
We supply hopper dryers and dehumidifying dryers, and we do not run your drying trial. So here is the honest limit: whether 65 °C for 4 hours reaches 0.05 % on your lot depends on bed depth and on how much air actually moves through the bed, and the only way to know is to sample at the dryer outlet and test it. A 500 mm bed dries slower than a 200 mm bed in the same machine, and nameplate airflow is measured with an empty hopper.
Two things we can do properly. We can size the air side against your consumption and the window above, and state the basis we used so you can check the arithmetic instead of trusting it. And we can tell you when a machine-side dryer is the wrong purchase because the plant air, not the dryer, is the problem — eight presses on one grade is a central drying project, while one press on a 4-hour cycle is not.
Send the grade and its sheet, the shot weight and cycle time, the number of machines, and whether you run regrind. The working volume and the dew point follow from those, and the numbers above are how we get there. Our range starts at machine-side hopper and dehumidifying dryers and goes up from there.